SPD Tech Circuit Protection Devices & Solutions
中文

Component Electronic Paste

· 5 min
PasteConductiveSilverThermalAdhesionCTE

Conductive / thermal / insulative electronic paste systems: silver paste, conductive adhesive, insulative thermal adhesive — curing mechanism, key properties (resistivity, adhesion, thermal) and the link to circuit protection (thermal stress, insulation).

Component electronic pastes (conductive / insulative) are three key materials for internal conductor interconnect, thermal path, and insulating fixation inside a device. Typical forms: screen-printed paste, dispensed adhesive paste, potted thermal adhesive.

Three paste types & curing

Type Filler Cure Typical use
Conductive paste Ag / Au / Pd / C + glass Glass melts 300–400 °C to bond Thick-film interconnect, SPD terminal fixation
Insulative thermal paste Al₂O₃ / AlN / BN + epoxy / silicone Resin thermal cure / RTV Power-device thermal interface, IGBT fixation
Conductive adhesive Ag / Au + epoxy / silicone Low-temp 80–150 °C thermal cure Wire-bond alternative, FPGA attach

Conductive paste silver + glass cures at 300–400 °C reflow: glass softens → wraps silver particles → glass chemically bonds to metal substrate (Cu / Al) → interconnect forms. Conductive resistivity is dominated by silver particle density and glass content (15–25% glass is optimal).

Key properties

  • Resistivity: conductive silver paste 10⁻³–10⁻⁵ Ω·cm (silver + glass), well above pure silver (1.6 × 10⁻⁶ Ω·cm); conductive adhesive 10⁻⁴–10⁻⁵ Ω·cm.
  • Adhesion: conductive paste ≥ 10 N/mm (measured shear); glass–metal chemical bond is the key.
  • Thermal conductivity: insulative thermal paste 0.5–3 W/mK (Al₂O₃ / AlN at 70–85% loading); conductive silver paste 100–250 W/mK (silver body).
  • Temperature: conductive paste reflow 300–400 °C, upper working limit 200–250 °C (glass long-term softening point).
  • Moisture: cured conductive paste < 0.5% (volume) absorption; long-term 85 °C/85% RH resistance drift < 10%.
  • SPD terminal fixation (MOV / GDT terminal leads): conductive paste reflow 300 °C replaces traditional tin soldering, avoiding thermal-shock damage to MOV grains; also provides mechanical fixation (10–50 N/mm shear).
  • IGBT / MOSFET fixation (power devices): insulative thermal paste (AlN-filled) as the thermal interface, replaces solder (solder grain coarsening / fatigue cracking at high temp), long-term 200 °C.
  • Thick-film SPD interconnect (ceramic-substrate MOV): conductive silver paste as resistor / capacitor thick-film material, co-fired with ceramic at 300 °C.
  • Isolation withstand: insulative thermal paste 10–30 kV/mm, IEC 61643-1 1500 V / 1 min power-frequency is mandatory for SPD potting + fixation.

Selection notes

  1. Conductive type: silver (low cost, thick-film) / gold (oxidation-resistant, wire-bond alt) / carbon (lowest cost, low-current only).
  2. Filler type: AlN (1.2–1.6 W/mK body) outperforms Al₂O₃ (0.2–0.4 W/mK), but AlN costs 3–5× more.
  3. Cure temperature: low-temp conductive adhesive (80–150 °C) for plastic / thin-film substrates; 300–400 °C reflow for ceramic / metal substrates.
  4. Adhesion: glass component must match substrate (Al-substrate → Al-glass, Cu-substrate → Cu-glass).
  5. Temperature: actual working temp + 50 °C margin; glass long-term softening is the key upper limit.

Common failures

Conductive paste incomplete reflow (300 °C too low / time too short, glass phase not fully softened), filler settling (silver / AlN sinks on substrate over long hot storage, conductor / thermal weakens on top), and moisture + silver-oxidation resistivity drift (85 °C/85% RH) are the top three — pick glass matching substrate + proper reflow profile to avoid them.